Effect of Pouring Temperature on Casting

2023-10-20
Defects easily caused by high-temperature pouring include burning sand, iron inclusion, shrinkage cavity, shrinkage porosity, hot crack, misfire, local oxidation, size unqualified, reactive porosity, and so on. The high pouring temperature can also cause the sand mold to expand, especially the gray iron casting with a complex sand core. When the pouring temperature ≥1420 °c, the waste products increase, and when the pouring temperature is 1460 °c, the waste products reach 50%. In production, the temperature of molten iron can be well controlled by induction furnace melting.

Possible defects at too low temperature

1)Manganese sulfide pore
This kind of blowhole is located below the surface of gray iron casting and often appears after machining. The diameter of the BLOWHOLE is about 2 ~ 6mm. Sometimes there is a little slag in the hole. Metallographic study shows that the defect is caused by MnS segregation and slag mixing, because of low pouring temperature and high Mn and s content in molten iron.

Such as content and appropriate MN content of 0.5% ~ 0.65% can significantly improve the purity of liquid iron, thus effectively prevent such defects.

2)Gas porosity in sand cores
Porosity and multi-porosity porosity is often caused by poor sand core venting. Because the core is usually hardened in the core box, this often leads to a lack of vent holes in the core. In order to form the vent hole, the core can be hardened after the additional drilling.

3)Liquid slag
After processing, small holes with a diameter of 1 ~ 3mm are found under the surface of gray iron castings. In some cases, there are only 1 or 2 small holes. The metallographic study showed that these holes appeared with a small amount of liquid slag, but no s segregation was found there. The results show that the defects are related to the pouring temperature. When the pouring temperature is higher than 1380 °c, the defects are not found in the castings. It is worth mentioning that the gating system’s design has not been changed to eliminate the defect, which can be attributed to the low pouring temperature and the formation of molten iron in the micro-reduction atmosphere.

The most common cause of low pouring temperature is that the molten iron has been transported and stayed in the ladle for a long time before pouring. The heat loss can be significantly reduced by using a ladle cover with an insulating material.


ABOUT  KEVA
Keva Casting is a professional casting company that focuses on Construction, Machinery, Automobile, Hardware, Pipeline and many other industries.
We provide top quality products with the best service based on our complete production chain including our own mold design, advanced production techniques, and full management of the supply chain. Keva Casting has two factories located in Zhucheng, China's Shandong province.
We use "shell molding", which is a new technique that has been developed in recent years.This new technique has simplified production procedures and reduced air pollution compared with traditional sand casting and investment casting. Shell making and core making are faster to ensure production in enormous quantities. The dimensions and surface finishing are satisfactory for all kinds of industrial requirements. Besides supplying our own formwork & scaffolding systems, our casting products also supply OEM services in various industries.

主站蜘蛛池模板: 台北县| 内黄县| 普洱| 商洛市| 乐昌市| 繁昌县| 隆安县| 峡江县| 弥勒县| 南和县| 习水县| 临城县| 汤阴县| 郯城县| 呼伦贝尔市| 峨眉山市| 普安县| 平山县| 嘉峪关市| 开阳县| 澄迈县| 桃园县| 上虞市| 阿克陶县| 堆龙德庆县| 资源县| 雅安市| 天长市| 中山市| 运城市| 虹口区| 白山市| 吴桥县| 凤翔县| 竹山县| 宁都县| 民乐县| 泰来县| 锦屏县| 新昌县| 芒康县|